        Yield strength: It is the yield limit when the metal material yields, that is, the stress that resists the slight plastic deformation. For metallic materials without obvious yield, the stress that produces 0.2% residual deformation is defined as its yield limit, which is called the conditional yield limit or yield strength. An external force greater than this limit will permanently deform the part and cannot be recovered.

        image.png

        experiment method

        There are generally two methods for measuring the upper and lower yield strengths: the graphic method and the pointer method.

        · Graphic method

        During the test, an automatic recording device was used to draw the force-chuck displacement diagram. It is required that the ratio of the force axis is less than 10N/mm2 per mm, and the curve must be drawn at least to the end of the yield stage. Determine the constant force Fe on the yield platform, the maximum force Feh before the force first falls in the yield stage, or the minimum force FeL that is less than the initial transient effect on the curve.

        The yield strength, upper yield strength and lower yield strength can be calculated according to the following formula:

        Yield strength calculation formula: Re=Fe/So; Fe is the constant force at yield.

        The formula for calculating the upper yield strength: Reh=Feh/So; Feh is the maximum force before the force drops for the first time in the yield stage.

        The calculation formula of the lower yield strength: ReL=FeL/So; FeL is the minimum force FeL less than the initial transient effect.

        · Pointer method

        During the test, the constant force when the pointer of the force measuring disc stops rotating for the first time or the maximum force before the pointer turns for the first time or the minimum force less than the initial instantaneous effect corresponds to the yield strength, upper yield strength, and lower yield strength, respectively.

        Guideline

        experiment method

        Pilot projects

        Test accuracy

        Room temperature tensile test

        Standard Test Methods for Tension   Testing of Metallic Materials

        ASTME8/E8M-13a

        Standard Test Methods and   Definitions

        for Mechanical Testing of Steel Products  

        ASTM A370-14

        Metallic materials -- Tensile   testing -- Part 1: Method of test at room temperature

        EN ISO6892-12009

        Metal material indoor tensile test   method

        GB/T228-2002

        Metallic material tensile test Test   method at room temperature

        JISZ2241-2011

        Metallic materials -Tensile testing   at ambient temperature

        AS 1391-2007

        Standard Test Methods for Tension   Testing Wrought and Cast Aluminum-and Magnesium-Alloy Products

        ASTM B557-14

        High temperature tensile test

        Standard Test Methods for Elevated   Temperature Tension Tests of Metallic Materials

        ASTME21-09

        Metallic materials -- Tensile   testing - Part 2: Method of test at elevated temperature

        ISO 6892-22011

        Metallic materials--Tensile testing   at elevated temperature

        GB/T 4338-2006

        High-temperature tensile test   method for steel materials and heat-resistant alloys

        JIS G0567-1998

        Metallic materials--Tensile testing   at elevated temperature

        AS 2291-2007

        Low temperature tensile test

        Metallic materials Low temperature   tensile test method

        GB/T 13239-2006

        Metallic materials Low temperature   test method

        ISO 15579:2000

        Yield strength testing and sample preparation requirements

        Normal temperature and high temperature stretching: 1. Wire and round bar samples: d≥10mm, length L≥200mm 3mm≤d≤10mm, length L≥200mm d≤3mm, length L≥1000mm (minimum wire 300mm, minimum bar 80mm ) 2. Rectangular sample: ≥16*200mm (L min 120mm) 3. Tubular sample: OD ≤ 30mm, L ≥ 300mm (min 150) OD> 30mm, general requirement L ≥ 300mm and OD ≤ 55mm, can be used for whole tube Stretching 4. The shrinkage rate of the cross section requires the length of the detection interval d ≥ 5mm.


        Online consultation

        Online consultation

        Recommend
        • Australian RCM certification

          Australian RCM certification

          Australian RCM certification

        • Label printer ANATEL certification

          Label printer ANATEL certification

          Label printers entering the Brazilian market, ANATEL certification is an essential passport! It is the recognition of the Brazilian Telecommunications Authority for the safety and compliance of electronic products, without which products cannot be legally sold.

        • Label printer SRRC certification

          Label printer SRRC certification

          SRRC certification is not only a guarantee of product compliance, but also a key to opening up the market.

        Yield strength test

        Yield strength: It is the yield limit when the metal material yields, that is, the stress that resists the slight plastic deformation.

        Get a quote
        主站蜘蛛池模板: 另类天堂天堂av| 亚洲最新版无码AV| 中日韩精品视频一区二区三区| 99re8免费视频精品全部| 久久综合给合综合久久| 特级无码毛片免费视频尤物| 成人视频XXxx| 久久精品国产只有精品66| 黄色大片一区二区中文字幕| 精品国产午夜理论片不卡精品| 亚洲欧洲一区二区福利片| 亚洲激情av| 亚洲中文字幕乱码av波多ji| 91色老久久精品偷偷蜜臀| 永泰县| 国产内射XXXXX在线| 区久久aaa片69亚洲| 韩国三级+mp4| 国产精品香蕉在线| 精品久久精品久久人妻| 国产高清在线精品一本大道| 美女黄18以下禁止观看| 精品av| 性欧美丰满熟妇xxxx性| 亚洲国产香蕉视频欧美| 晋中市| 欧美精品在线免费| 亚洲精品字幕在线观看| 国产精品无码永久免费A片| 亚洲丶国产丶欧美一区二区三区| 乱伦网址| 国语自产精品视频在线区| 韩国青草无码自慰直播专区| 美女久久久久久久久久久| 玩弄少妇人妻中文字幕| 国产精品久久久久久影视不卡| 亚洲 自拍 偷拍 另类综合图区| 三级无码在钱av无码在钱| 日本免费一区二区三区四区五六区| 熟女五码SV| а√天堂最新版在线资源|